- 3004 Aluminum Coil Specifications
- 3004 Aluminum Coil Advantages
- Features of 3004 Aluminum Coil
- Equivalents of AA 3004
- 3004 Aluminum Coil Manufacturer Product Quality
- Typical Mechanical Properties Data of Aluminum 3004
- Aluminum Coil 3004 Mechanical Properties
- 3004 Aluminum Coil More Informations
- 3004 Aluminum Coil Physical Data
- 3004 Aluminum Coil Tolerance on Forms and Dimensions
- 3004 Aluminum Coil Applications
- 3004 Aluminum Chemical Composition
- 3004 Aluminum Coil VS 3003 Aluminum Coil
- 3004 Aluminum Coil Related Questions
- 3004 Aluminum Coil Packaging Handling Storage
3004 aluminum coil is a common aluminum alloy coil, mainly composed of aluminum, magnesium and a small amount of other alloying elements. It has excellent corrosion resistance, processability and welding performance, and is often used in the manufacture of industrial parts such as automobile bodies, fuel tanks, tanks, and building shells.
- Processing: As an aluminum alloy, 3004 aluminum coil has excellent processability.
- Heat treatment: Like 3003, 3004 aluminum coil cannot be heat treated.
- Welding: This alloy has good weldability.
The performance and application range of 3004 aluminum coils are also affected by factors such as specifications, conditions, and surface treatments. Which specification and state of 3004 aluminum coil to choose should be selected according to actual use requirements and process requirements.
3004 Aluminum Coil Specifications
- Thickness : 0.2mm - 6.0mm
- Width : 100mm - 2600mm
- Length : can be customized according to customer needs
- Status : H14, H16, H18, H19, H22, H24, H26, H28, H32, H34, H36, H38
It should be noted that the specifications of 3004 aluminum coils produced by different manufacturers may be different, and the specific specifications need to be confirmed with the manufacturer.
3004 Aluminum Coil Advantages
- Good weldability
- High corrosion resistance
- Good plasticity
- Formability and solubility are also quite good
- Medium strength
The main disadvantage of 3004 aluminum coil is that it is not heat treatable.
Features of 3004 Aluminum Coil
- 1.3004 aluminum alloy can be cold worked (but not heat treated like other types of aluminum alloys) to produce a tempered state with higher strength but lower ductility.
- 2.3004 aluminum is usually rolled and extruded (for making beverage cans), but is not usually forged. As a forging alloy, it is not used for casting.
- 3.3004 aluminum coil has higher plasticity in the annealed state, better plasticity in the semi-cold hardened state, and lower plasticity in the cold hardened state. The anodized 3004 aluminum plate surface has enhanced corrosion resistance and can present a rich and colorful color.
Equivalents of AA 3004
UNS A93004, ISO AlMn1Mg1, Aluminium 3004, AA3004, Al3004
3004 Aluminum Coil Manufacturer Product Quality
- Advanced production technology and equipment : Adopt advanced production technology and equipment to produce high-quality 3004 aluminum coils to ensure the accuracy and stability of the thickness, width and surface quality of aluminum coils.
- High-quality Raw Materials : Use high-purity, low-impurity aluminum as raw materials to ensure the physical properties and corrosion resistance of aluminum coils.
- Strict Quality Control : Strictly control every link in the whole production process, including material procurement, production process, quality inspection and other aspects.
- Perfect after-sales Service : provide perfect after-sales service, including responding to and solving customer problems in a timely manner.
Typical Mechanical Properties Data of Aluminum 3004
Alloy-Temper |
Tensile Strength (ksi) |
Yield Strength (ksi) |
Elongation (%) |
3004-O | 26 | 10 | 19 |
3004-H34 | 39 | 29 | 5 |
3004-H38 | 41 | 36 | 4 |
Aluminum Coil 3004 Mechanical Properties
Temper | Specified Thickness(in) | Tensile Strength - KSI | Elongationin 2 inches % | |||
Ultimate | Yield | |||||
Min | Max | Min | Max | |||
H22/32 | 0.017 - 0.019 | 28 | 35 | 21 | - | 1 |
H22/32 | 0.020 - 0.031 | 28 | 35 | 21 | - | 3 |
H22/32 | 0.032 - 0.050 | 28 | 35 | 21 | - | 4 |
H22/32 | 0.051 - 0.113 | 28 | 35 | 21 | - | 5 |
H22/32 | 0.114 - 2.000 | 28 | 35 | 21 | - | 6 |
H24/34 | 0.009 - 0.019 | 32 | 38 | 25 | - | 1 |
H24/34 | 0.020 - 0.050 | 32 | 38 | 25 | - | 3 |
H24/34 | 0.051 - 0.113 | 32 | 38 | 25 | - | 4 |
H24/34 | 0.114 - 1.000 | 32 | 38 | 25 | - | 5 |
H26/36 | 0.006 - 0.007 | 35 | 41 | 28 | - | - |
H26/36 | 0.008 - 0.019 | 35 | 41 | 28 | - | 1 |
H26/36 | 0.020 - 0.031 | 35 | 41 | 28 | - | 2 |
H26/36 | 0.032 - 0.050 | 35 | 41 | 28 | - | 3 |
H26/36 | 0.051-0.162 | 35 | 41 | 28 | - | 4 |
H28/38 | 0.006 - 0.007 | 38 | - | 31 | - | - |
H28/38 | 0.008 - 0.019 | 38 | - | 31 | - | 1 |
H28/38 | 0.020 - 0.031 | 38 | - | 31 | - | 2 |
H28/38 | 0.032 - 0.050 | 38 | - | 31 | - | 3 |
H28/38 | 0.051 - 0.128 | 38 | - | 31 | - | 4 |
O | 0.006 - 0.007 | 22 | 29 | 8.5 | - | - |
O | 0.008 - 0.019 | 22 | 29 | 8.5 | - | 10 |
O | 0.020 - 0.031 | 22 | 29 | 8.5 | - | 14 |
O | 0.032 - 0.050 | 22 | 29 | 8.5 | - | 16 |
O | 0.051 - 0.249 | 22 | 29 | 8.5 | - | 18 |
O | 0.250 - 3.000 | 22 | 29 | 8.5 | - | 16 |
3004 Aluminum Coil More Informations
Property | Description |
Principal Design Features | This is an alloy of aluminum with magnesium and manganese. It is strengthened (hardened) by cold work only as it does not respond to heat treatment, other than annealing. |
Machinability | The machinability of this alloy is considered to be excellent, especially in the hard temper. As is typical of the aluminum alloys an oil lubricant should be used for machining, although light cuts may be done dry. |
Forming | AL 3004 is easily formed by either cold or hot working with conventional tooling. |
Welding | The alloy is weldable by the standard methods. Best results are obtained by use of TIG or MIG welding with the same alloy as filler rod. |
Heat Treatment | Heat treatment has no effect upon this alloy. It may be annealed after cold working however. |
Hot Working | The hot working range (as for forging) is 260°C to 483°C. In that range the alloy is easily hot worked. |
Cold Working | Cold working capability of this alloy is good: it can readily be cold worked up to a 75% reduction of area by conventional methods. Working beyond the 75% reduction requires an intermediate anneal. |
Annealing | Annealing, during or following cold working, is done at 344°C, allowing adequate time for thorough heating, followed by air cooling. |
Aging | Not applicable to this alloy. |
Hardening | Cold working is the only means of producing the harder (H) tempers of this alloy. |
3004 Aluminum Coil Physical Data
Property | Value |
Density (20°C) | 2, 720 kg/m³ |
Melting Point | 629°C |
Thermal Expansion (20°C ~ 100°C) | 23.2 x 10⁻⁶ /K |
Modulus of Elasticity | 70 GPa |
Thermal Conductivity (Temper O) | 162 W·m⁻¹·K⁻¹ |
Electrical Resistivity (Temper O) | 0.041 x 10⁻⁶ Ω·m |
Conductivity (Temper O) | 42 %IACS |
Magnetic Performance | No |
Color | Silver |
Odour | No |
3004 Aluminum Coil Tolerance on Forms and Dimensions
3004 Aluminum Coil Thickness Tolerance
Thickness | Width ≤1000mm | Width >1000-1250mm | Width >1250-1600mm | Width >1600-2000mm |
≥ 0.2-0.4mm | ± 0.02mm | ± 0.04mm | ± 0.05mm | ± 0.05mm |
> 0.4-0.5mm | ± 0.03mm | ± 0.04mm | ± 0.05mm | ± 0.06mm |
> 0.5-0.6mm | ± 0.03mm | ± 0.05mm | ± 0.06mm | ± 0.07mm |
> 0.6-0.8mm | ± 0.03mm | ± 0.06mm | ± 0.07mm | ± 0.08mm |
> 0.8-1.0mm | ± 0.04mm | ± 0.06mm | ± 0.08mm | ± 0.09mm |
> 1.0-1.2mm | ± 0.04mm | ± 0.07mm | ± 0.09mm | ± 0.10mm |
> 1.2-1.5mm | ± 0.05mm | ± 0.08mm | ± 0.10mm | ± 0.11mm |
> 1.5-1.8mm | ± 0.06mm | ± 0.09mm | ± 0.11mm | ± 0.12mm |
> 1.8-2.0mm | ± 0.08mm | ± 0.10mm | ± 0.12mm | ± 0.13mm |
> 2.0-2.5mm | ± 0.10mm | ± 0.12mm | ± 0.15mm | ± 0.16mm |
> 2.5-3.0mm | ± 0.12mm | ± 0.15mm | ± 0.17mm | ± 0.18mm |
> 3.0-4.0mm | ± 0.14mm | ± 0.18mm | ± 0.20mm | ± 0.22mm |
> 4.0-6.0mm | ± 0.18mm | ± 0.22mm | ± 0.24mm | ± 0.25mm |
3004 Aluminum Coil Width Tolerance
Thickness | Width ≤300mm | Width >300-500mm | Width >500-1250mm | Width >1250-1650mm | Width >1650mm |
≥ 0.2-0.6mm | ± 0.4mm | ± 0.6mm | ± 1.5mm | ± 2.5mm | ± 3.0mm |
> 0.6-1.0mm | ± 0.5mm | ± 0.8mm | ± 1.8mm | ± 2.8mm | ± 3.3mm |
> 1.0-2.0mm | ± 0.7mm | ± 1.0mm | ± 2.0mm | ± 3.0mm | ± 3.5mm |
> 2.0-3.0mm | ± 1.0mm | ± 1.5mm | ± 2.5mm | ± 3.5mm | ± 4.0mm |
> 3.0-6.0mm | ± 1.5mm | ± 2.0mm | ± 3.0mm | ± 4.0mm | ± 5.0mm |
3004 Aluminum Coil Length Tolerance
Thickness | Length ≤1000mm | Length >1000-2000mm | Length >2000-3000mm | Length >3000mm |
≥ 0.2-3.0mm | ± 3mm | ± 4mm | ± 6mm | ± 8mm |
> 3.0-6.0mm | ± 4mm | ± 6mm | ± 8mm | ± 10mm |
3004 Aluminum Coil Flatness Tolerance
Thickness | Total Deviation | On Length | On Width | Partial Deviation |
≥ 0.2-0.5mm | By agreement | By agreement | By agreement | By agreement |
> 0.5-3.0mm | ≤ 0.4% | ≤ 0.5% | ≤ 0.5% | ≤ 0.5% |
> 3.0-6.0mm | ≤ 0.3% | ≤ 0.4% | ≤ 0.4% | ≤ 0.4% |
3004 Aluminum Coil Lateral Curvature Tolerance
Width | ≤1000mm | >1000-2000mm | >2000-3500mm | >3500mm |
≤300mm | ≤ 2.0mm | ≤ 4.0mm | ≤ 8.0mm | - |
>300-600mm | ≤ 1.5mm | ≤ 3.0mm | ≤ 5.0mm | - |
>600-1000mm | ≤ 1.0mm | ≤ 2.0mm | ≤ 4.0mm | ≤ 5.0mm |
>1000-2000mm | - | ≤ 2.0mm | ≤ 4.0mm | ≤ 5.0mm |
>2000mm | - | - | ≤ 4.0mm | ≤ 5.0mm |
3004 Aluminum Coil Squareness Tolerance
Length | ≤1000mm | >1000-1500mm | >1500-2000mm | >2000mm |
≤1000mm | ≤ 4.0mm | - | - | - |
>1000-2000mm | ≤ 4.0mm | ≤ 5.0mm | - | - |
>2000-3000mm | ≤ 5.0mm | ≤ 5.8mm | ≤ 7.0mm | - |
>3000-5000mm | ≤ 6.0mm | ≤ 7.0mm | ≤ 8.0mm | ≤ 10.0mm |
3004 Aluminum Coil Applications
Lamp material, louver material, heat sink, liquid crystal back panel material, bottle cap material, aluminum base material for color coating, etc.
- Building and construction : 3004 aluminum coils are used for building exterior wall panels, roof panels, ceilings, wall panels and skylights, etc.
- Electronics : 3004 aluminum coils are used to manufacture electronic product casings, heat spreaders and heat sinks, etc.
- Packaging : 3004 aluminum coils are used to manufacture various packaging, such as beverage cans, food cans and pharmaceutical cans.
- Automotive and transportation : 3004 aluminum coils are used in the manufacture of automotive parts such as doors, roofs and hoods.
- Furniture and home decoration : 3004 aluminum coils are used in the manufacture of various furniture and home decoration products such as tables, chairs, lamps and decorative panels, etc.
- Other applications : 3004 aluminum coils are also used in shipbuilding, chemical equipment, household appliances, mechanical equipment and manufacturing handicrafts and other fields.
3004 Aluminum Chemical Composition
element | Si | Fe | Cu | Mn | Mg | Cr | Zn | Ti | Others-Each | Others Total | Al Min |
3004 | 0.30 | 0.7 | 0.25 | 1.0-1.5 | 0.8-1.3 | – | 0.25 | 0.25 | 0.05 | 0.15 | Remainder |
3004 Aluminum Coil VS 3003 Aluminum Coil
Both 3004 aluminum coil and 3003 aluminum coil are aluminum alloy coils, which are often used in the manufacture of industrial components such as vehicle bodies, tanks, building shells, and fuel tanks.
Chemical Composition
3004 aluminum coils contain 1% magnesium, while 3003 aluminum coils do not contain magnesium. Therefore, 3004 aluminum coil has better corrosion resistance, weldability and processing performance than 3003 aluminum coil.
Strength
The strength of 3004 aluminum coil is slightly higher than that of 3003 aluminum coil, but its plasticity is slightly lower. Therefore, 3004 aluminum coils can be selected for occasions that require high strength but less plasticity; and 3003 aluminum coils can be selected for occasions that require high plasticity but less strength.
3004 Aluminum Coil Related Questions
Question | Answer |
What is the difference between 3003 and 3004 aluminum? | The main difference is in alloy composition; 3004 has higher manganese content for improved strength and corrosion resistance compared to 3003. |
What is aluminum alloy Al 3004? | Aluminum alloy 3004 is used in beverage cans and containers due to its strength, formability, and corrosion resistance. |
Is 3004 aluminum weldable? | Yes, 3004 aluminum is weldable using conventional methods such as MIG and TIG welding. |
Is 3003 aluminum heat treatable? | No, 3003 aluminum is not heat treatable; its properties are set during casting and cannot be changed by heat treatment. |
Can 3004 Aluminum Coil Be Anodized? | Certain types of aluminum alloy react better to anodization than others. Aluminum coil 3004 contains manganese, so it can be anodized. However, the manganese typically causes discoloration during the anodization process. |
3004 Aluminum Coil Packaging Handling Storage
Category | Description |
Package | Packed in waterproof Kraft, fastened by steel straps on wood pallets, suitable for handling, loading and unloading from the trunks or containers, suitable for export ocean forwarding. |
Handling | Prevent the goods hurting the people who are moving, loading, unloading, especially pay attention to the rolling and dropping for the coils. |
Storage | Stored in indoor area on plain floor, free away from moisture, water, snow, animal oils and dye wastes, avoid storing with acid or basic chemical goods. |